Wednesday, 18 August 2021

Observations on Some Suggestions about Annealing

There are writings from a teacher attempting to make glass fusing simple.  Unfortunately, glass physics and chemistry are very complicated.  Attempting to avoid these complications leads to failures and other difficulties as the practitioner progresses. 

Proper annealing is one of the fundamentals to achieving sound kilnforming results.  Some suggestions have been made by a widely followed person to “simplify” the understanding of the annealing process.  Discussion of the meaning and importance of annealing can be found in many places, including here.  

Annealing temperatures
It has been suggested that the annealing temperatures can be inferred from the CoE of the glass that is being used. Discussion of what CoE is and is not can be found here and here.


Annealing temperatures are not directly related to the expansion coefficient (CoE) of the glass.  This can be shown from the published annealing temperatures for different glasses organised by presumed CoE:
·        “CoE96”: Wisssmach 96 - anneal at 482°C;  Oceanside - anneal at 515°C
·        “COE94”: Artista - anneal at 535°C
·        “CoE 93”: Kokomo - anneal between 507°C and 477°C – average 492°C
·        “CoE 90”: Bullseye - anneal at 482°C; Wissmach90 - anneal at 482°C; Uroboros FX90 - anneal at 525°C
·        “CoE 83”:
o   Pilkington (UK) float - anneal at 540°C;
o   typical USA float - anneal at 548°C;
o   Typical Australian float - anneal between 505°C and 525°C, average 515°C

This shows there is no direct relationship between CoE and annealing temperature.  Do not be tempted to use a CoE number to indicate an annealing temperature.  Go to the manufacturer’s web site to get the correct information.


Temperature equalisation soak
Annealing for any glass can occur over a range of temperatures.  The annealing point is the temperature at which the glass can most quickly be annealed.  However, the glass cannot be annealed if it is not all at the same temperature throughout the substance of the glass.  It has been shown through research done at the Bullseye Glass Company that a temperature difference of more than 5°C will leave stress within the glass piece. To ensure good annealing, adequate time must be given to the temperature equalisation process (annealing). 

From the Bullseye research the following times are required for an adequate anneal soak:
6mm /   1/4"            60 minutes
[9mm /  3/8"           90 minutes]
12mm  / 1/2"          120 minutes
[15mm  /   5/8"       150 minutes]
19mm   / 3/4"         180 minutes

[ ] = interpolated from the Bullseye chart for annealing thick slabs


Anneal Cooling
There are suggestions that a “second anneal” can be used on important pieces.  Other than observing that all pieces are important to the maker, the suggestion should be investigated.  On looking into the idea, it is essentially a second soak at 425°C, which is slightly below the strain point, rather than controlled cool from the anneal soak temperature.

It is reported that the Corning Museum of Glass considers 450°C as the lower strain point – the temperature below which no further relief of strain is possible.  This means that any secondary soak must occur above 450°C rather than the suggested 425°C. Such a soak is unnecessary if the appropriate cooling rates are used. 

Cooling Rate
Except in special circumstances, the cooling rate needs to be controlled as part of the annealing process.  Soaking the glass at the anneal is not the completion of the annealing.  Most practitioners follow the practice of choosing a slow rate of cooling from the annealing soak to some point below the strain point rather than a rapid one with a soak at the strain point temperature.

Annealing is not just the soak time (which is there to equalise the temperature), it is about the rate of the annealing cool too. The rate at which you cool is dependent on the thickness of the glass piece and whether it is all of one thickness or of variable thicknesses.

Even thickness
                                         Cooling rate
Dimension      time (mins)     1st 55°C   2nd 55°C
6mm              60                 83°C       150°C
9mm              90                 69°C       125°C
12mm            120                55°C       99°C
15mm            150                37°C       63°C
19mm            180                25°C       27°C

The “first 55°C” and the “second 55°C” refer to the temperature range below the chosen annealing temperature.  So, if you choose to anneal at 515°C, the “first 55°C” is from 515°C to 460°C and the “second 55°C is from 460°C to 405°C.  If you choose 482°C as the annealing temperature, the “first 55°C” is from 482°C to 427°C and the “second 55°C from 427°C to 372°C.

Tack fused/ uneven thickness
If your piece is tack fused, you need to treat the annealing rate and soak as though it were twice the actual total thickness. This gives the following times and rates:

Tack fused
Dimension (mm)                                Cooling rate
Actual     Calculated       time (mins)     1st 55°C   2nd 55°C
6            12                 120                55°C       99°C
9            18                 150                37°C       63°C
12          25                 180                25°C       27°C
15          30                 300                37°C       63°C
18          38                 360                7°C         12°C

Contour fusing required firing as though the piece were 1.5 times thicker.  Sharp tack or laminating requires 2.5 times the the actual thickness.

Fusing on the floor of the kiln
There is a further possible complication if you are doing your fusing on the kiln floor, or a shelf resting on the floor of the kiln.  In this case you need to use the times and rates for glass that is at least 3mm thicker than the piece actually is. 

Thus, a flat 6mm piece on a shelf on the floor would use the times and rates for 9mm: anneal soak for 90 minutes, anneal cool at 69°C to 427°C and then at 124°C to 371°C.  It would be safest if you continued to control the cooling to room temperature at no more than 400°C per hour.

But if it were a tack fused piece of a total of 6mm you would use the times and rates for 18mm.  This is using the rates for twice the total thickness plus the additional 3mm for being on the base of the kiln.  This gives the times and rates as being an anneal soak of 360 minutes and cooling rates of 7°C to 427°C and 12°C to 370, followed by 40°C per hour to room temperature.  Any quicker rates should be tested for residual stress before use.


Source for the annealing and cooling of fused glass
These times and rates are based on the table derived from Bullseye research, which is published and available on the Bullseye site.   It is applicable to all fusing glass with adjustments for differing annealing soak temperatures.


Annealing over multiple firings
It has been recommended by this widely followed person that the annealing soak should be extended each time subsequent to the first firing.  I am uncertain about the reasoning behind this suggestion. But the reasons for discounting it are related to adequate annealing and what is done between firings.

If the annealing is adequate for the first firing, it will be adequate for subsequent firings unless you have made significant alterations to the piece.  If you have added another layer to a full fused piece, for example and are using a tack fuse, you will need to anneal for longer, because the style and thickness have been altered.  Not because it is a second firing.  If you are slumping a fired piece, the annealing does not need to be any different than the original firing.

The only time the annealing needs to be altered is when you have significantly changed the thickness of the piece, or the style of fusing (mainly tacking additional items to the full fused piece).  This is when you need to look at the schedules you are planning to use to ensure your heat up is slow enough, that your annealing soak is long enough, and the cool slow enough for the altered conditions.


Determining the annealing point of unknown glass
You don’t have to guess at the annealing temperature for an unknown glass.  You can test for it.  It is known as the slump point test.

This test gives the softening point of the glass and from that the annealing point can be calculated.  This test removes the guess work from choosing a temperature at which to perform the anneal soak. The anneal temperature is important to the result of the firing.  This alone makes this test to give certainty about the annealing temperature worthwhile.

You can anneal soak at the calculated temperature, or at 30°C below it to reduce the anneal cool time.  This is because the annealing can occur over a range of temperatures.  The annealing occurs slowly at the top and bottom of the range. But is at least risk of "fixing in" the stress of an uneven distribution of temperature during the cool when the annealing is done at the lower end of the range.



Do not be fooled into thinking that CoE determines annealing temperatures.  Use published tables, especially the Bullseye table Annealing for Thick Slabs to determine soak times and cooling rates.  Use the standard test for determining the softening and annealing points of unknown glasses.


Further information is available in the ebook Low Temperature Kiln Forming.