Wednesday, 28 August 2024

Visible Devitrification

"Why does devitrification appear on slumped pieces?"

A brief explanation 

Scientific research in developing a glass matrix to support bone grafts gives some information.  This kind of glass matrix requires to be strong.  Development showed that devitrification weakens the matrix.  The crystals in a matrix are not as strong as the amorphous glassy state.  So, devitrification needs to be avoided.

The research to avoid devitrification showed that it begins at about 600˚C/1110˚F.  It only begins to become visible above 700˚C/1300˚F.  The process developed was to introduce a “foaming” agent.  The process fired slowly to 600˚C/1110 ˚F and then quickly to 830˚C/ 1530˚F.  It left a strong open matrix around which bone can grow. Although the research used float glass, it is also a soda lime glass, just as fusing glasses are.  The formation of devitrification begins at the same temperature for fusing glasses as for float.

The result of this medical research shows that devitrification begins on glass before it is visible. Devitrification is cumulative. A little becomes greater with another firing.  This is so even with good cleaning between firings. The new devitrification builds on the previous.  It does this from 600˚C/1110 ˚F.

A subsequent firing can continue this devitrification to the point where it is visible. This can happen, although the temperature at which we can see it after one firing has not been reached.  This continued devitrification at low temperatures can become great enough to be visible at the end of one or multiple slumps.

Credit: Bullseye Glass Co.

What can we do?

Clean all the glass before every firing very well.

·         Avoid mineralised water.

·         Final clean with isopropyl alcohol.

·         Polish dry at each stage with white absorbent paper.

 

Soak longer at lower temperatures.

·         Use longer soaks to achieve the slump.

·         Keep the temperature low.

·         Observe the progress of the firing with quick peeks.

 

Use slower ramp rates.

·         Slower rates enable the heat to permeate the glass.

·         Enables a lower slump temperature.

 

If there is any hint of devitrification after the first firing,

·      use a devitrification spray, or

·      provide a new surface.

    • o   remove the surface by abrasion on sandblasting,
    • o   cap with clear, or
    • o   cover whole surface with a thin layer of clear powder.

·      Fire to contour fuse to give a new smooth surface.

·      Clean very well and proceed to slump.