Wednesday 21 August 2024

Slower Ramps on Additional Firings

"Every time you fire a previously fired piece you need to slow down."

This is not accurate. If you have not changed anything significant, the annealing does not need to be extended.  The clearest example is a fire polish.  Nothing has been added. The physics and chemistry of the piece have not changed.  If only confetti or a thin frit/powder layer is added, nothing significant for scheduling has been added.  As nothing significant has changes the annealing used in the previous firing can be used again.

Of course, you do need to slow the ramp up rates on the second firing.  This is because you are firing a single thicker piece.  On the first firing, the pieces are individual and can withstand slightly faster rates. But on third and subsequent firings, if nothing significant has been changed, there is no need to slow rates further.

There is a post which describes this further.



"When adding more thickness more time is needed."

This is the occasion when the annealing soak needs to be extended.  Placing a full sheet of clear glass on the bottom, or less usually, the top, and taken to a full fuse, requires slower ramp rates.   The annealing time for a full fuse can be taken directly from the annealing tables for thick slabs.  

The fusing profile for any additional items has a strong affect on the length of the annealing soak.  If the glass is now of uneven thicknesses, and greater care in assigning ramp rates is needed.  The profile for the piece also determines the amount of additional annealing time required.  A sharp tack of a single additional layer will require annealing as for 2.5 times the total height of the piece at the start or the firing. A rounded tack will need two times and a contour fuse will require 1.5 times.  A full fuse can be carried out for the new total height of the piece without any multiplying factors.

 If the intention with multiple firings is to achieve a variety of profiles within one piece, a slightly different approach is required.  A blog post here describes the process.


The general approach to multiple firings is that unless there are changes to the thickness or profile of the glass, no changes in annealing time is required.  

 

Wednesday 14 August 2024

Slow Rates to Annealing

"I have seen recommendations for slower than ASAP rates from the top temperature, but most schedules say 9999 or ASAP.  Which is right?"

Slow drops in temperature from top to annealing temperatures risk devitrification. Accepted advice is to go ASAP to annealing temperature to avoid devitrification forming.

Breaks do not occur because of a too rapid drop from top temperature to annealing. The glass is too plastic until the strain point has been passed to be brittle enough to break. On the way down that will be below an air temperature of 500˚C/933˚F.

credit: ww.protolabs.com


Different kilns cool from top temperature at different rates. Ceramic kilns are designed to cool more slowly and may need assistance to cool quickly.  This is usually by opening vents or even the door or lid a little. Glass kilns are designed to lose temperature relatively quickly from high temperatures. They do not need a crash cooling as ceramic kilns may need in certain circumstances.  Of course, crash cooling may be necessary for some free drops and drapes.

The length of the soak at annealing is determined by the effective thickness of the piece.  Tack fusing needs to be annealed for thickness as a factor of 1.5 to 2.5, depending on profile.

The extent to which you control the cooling to room temperature after the anneal soak is dependent on the calculated thickness of the piece you are cooling. The objective is to keep the internal temperature differential to 5˚C/10˚F or less to avoid expansion/ contraction differences that are great enough to break the piece. Those rates are directly related to the required length of the anneal soak.  Those rates can be taken from the Bullseye chart for Annealing Thick SlabsThe Fahrenheit version is is available too.

An example.  If you have a 2 layer base with 3 layers (=15mm) stacked on top for a rounded tack fuse, you need to fire as for at least 30mm. This will require controlled cooling all the way to room temperature.

  • ·        The rate to 427˚C /800˚F will be19˚C /34˚F
  • ·        The rate to 370˚C /700˚F will be 36˚C /65˚F
  • ·        The final rate 120˚C /216˚F to room temperature.

You may need to wait a day before any coldworking. An example from my experience shows the necessity.  I checked a piece for stress a few hours after removing the piece from the kiln when it felt cool to the touch. It puzzled me that stress showed, although it didn't on similar pieces.  The next morning, I went to check if I misunderstood the reading. Now, a full 15 hours after coming out of the kiln, there was no stress.  The example shows that the glass internally is hotter than we think. And certainly, hotter than the air temperature.

In the temperature regions above the strain point, the glass needs to be cooled quickly. In the annealing region and below the glass needs to be cooled slowly.

More information is available in the eBook Low temperature Kilnforming.  This is available from Bullseye or Etsy

Wednesday 7 August 2024

Longer Soak or Higher Temperature?

 ‘Is it better to extend the soak or add more firing time when the firing program isn’t quite enough? What are the meanings of “soak,” “hold,” “ramp,” “working temperature” and “top temperature”?’  

Let’s start with some of the terms.

Soak” and “hold” have the same meaning in scheduling.  Schedules are made up of a series of linked segments.  Each segment contains a rate, temperature, and time.  The time is often called a “hold” in the schedules.  That time can have several effects.  It can allow enough time for a process, such as slumping, to be accomplished.

Although “soak” is entered into the schedules in the same way as a hold, it has a different concept behind it.  The hold when used as a soak allows the set temperature to permeate the whole thickness of the glass.  An example is in annealing. An annealing hold/soak is set.  This is to allow the glass to become the same temperature throughout. 

The ramp is the rate at which the controller is set to increase/decrease the temperature.  This is normally the first element in the segment.

Top” and “Working” temperature are the same thing.  It is the temperature at which the desired effect is achieved.  They have slightly different nuances.  Top temperature is normally considered as a point where the desired profile will be achieved in a few minutes.  The working temperature is also that, but includes the idea that it will take time for the effect to be achieved.



Which should you alter first – soak time or temperature?

Most important is that you alter only one at a time.  If you alter the two elements at the same time, you do not know which was the cause of the result.

In general, you lengthen the soak if the effect is not achieved at the temperature and in the time set.  There are two reasons for this.  Glass has fewer problems at lower temperatures.  Secondly, the controllers are set up in such a way that it is easy to extend the time. Check your manual for the key sequence to extend the time.  It is more difficult to alter the temperature during a firing. 

To determine if you need more time, you peek into the kiln as the kiln approaches the top temperature.  If the profile has not been achieved by the time set at your working temperature, you enter the combination of keys to keep the kiln at the top temperature until you see the effect you want.  Then enter the combination of keys to skip to the next segment.


Whether you alter time or temperature, depends on what you are doing.  Soak plus temperature equal heat work.  With heat work you can accomplish the same effect at lower temperatures.  It may be that taking more time (usually slower ramp rates) to get to the same or lower temperature, will give the results desired.

For slumping, draping and other low temperature processes extending the hold/soak is appropriate. It reduces the amount of marking that is created by the mould or surface supporting the glass.

When tack, contour, or full fusing, you should be aiming to finish the work in about 10 minutes. Soaking/holding significantly longer increases the risk of devitrification.

For high temperature processes such as pot and screen melts and some flows, increasing the temperature is probably the right thing to do, to avoid the devitrification possibilities of long holds of open face high temperature work.

These can only be guidelines.  Your instincts and experience will help you determine which is the right thing to do in the circumstances.

 

Wednesday 31 July 2024

Placing of Pieces in the Kiln

 Distance from Sides of Kiln

 

"Is there a rule of thumb for interior size of kilns and piece size? (i.e., “allow for X inches between the piece and kiln walls on all sides”).  I’m thinking about how to determine piece size limitations when shopping for a kiln."

I don’t know of a formula, or rule of thumb, to determine the amount of space required between the glass and the kiln walls.

I have only been able to determine the spacing required after I have purchased the kiln.  Each kiln has different characteristics. 

The most obvious is whether the kiln is fired from the side or from the top.  More space is required with side fired kilns.  The radiant heat from the elements tends to heat the edges of the glass before the centre becomes equally hot. This requires more space or baffles between the elements and the glass.

Top fired,  with enough distance to get even distribution of heat

Side fired. Red arrows indicate the important infrared heating.
Blue arrows indicate the less effective ambient heat.


There is less concern about uneven heating with top fired kilns.  But as each kiln is different, you must test the heat distribution around the kiln.  Bullseye Tech Note #1 has a good method.  This will show where the temperature is less than the rest of the shelf.

In general, rectangular kilns are cooler in the corners.  Round kilns do not have the same characteristic, but may still have uneven temperatures, due to the configuration of the elements.  Smaller kilns seem to have more even temperatures than large kilns, which tend to be cooler along the sides.  Kilns with a ring element below the shelf seem to have the most even distribution of temperature.

I had a large kiln 2 metres by 1 metre which had a requirement of 50mm/2” from the edge to even the temperature.  A recently purchased 50cm square kiln has almost perfectly even temperatures across the whole shelf.

[The illustration is taken from the ebook Low Temperature Kilnforming, available from Bullseye and Etsy.]

The required glass distance from the side will depend on side or top elements and size but no formula is available.  Testing for heat distribution is necessary once you have the kiln.

Wednesday 24 July 2024

Changing size in Slumping

 “I have full fused a single piece of glass with a few small pieces on top.  I thought it would shrink some as I had been told, but it maintained its size and still fit the mold for slumping.” 

I believe the enquirer is talking about a single layer circle changing size at full fuse.  Dog boning is much less evident in circles than rectangles.  The glass retreats evenly all along the edge.  This gives the appearance of retreating less than rectangles.  The absence of any big change in size may also result from thinning of the centre.  The amount of size change will be affected by the temperature of the full fuse too.  In this case there were additions which will have resisted any tendency to shrink.

Lower top temperatures, more rapid ramp rates to the top, and shorter holds will have the effect of limiting the movement of glass toward 6mm thick.

credit: Bullseye Glass Co



The viscosity of glass at full fuse is enough for it to attempt to pull up to 6mm. At casting temperatures, the viscosity is so low that 6mm of glass spreads out.  Temperature affects viscosity.

 

At slumping temperatures (620˚C - 680˚C / ca.1150˚F - 1260˚F), the viscosity high enough that the dimensions of a circle do not change. A circular piece of 3mm glass held at slumping temperatures does not change dimension.  It may, if held long enough take on a kind of satin sheen, rather than a fire polish.  But the viscosity  is low enough to allow the glass to form to the mould, given sufficient time. The resulting slumped piece will appear to be smaller than the mould. If you measure the piece around its outside curve, you will find the distance is almost the same as the diameter of the blank. 


 

Changing size on a single layer piece is dependent on the temperature and heat work applied to the piece.

Wednesday 17 July 2024

Bowl Split Analysis


The visual evidence relating to this enquiry is a sharp-edged break through the middle of the slumped piece. The two parts have slumped separately, and seem attached at the rim, leaving the middle opened.  A moderate slumping temperature was used to fire the piece at the bottom of a stacked kiln load.

This is used as an example of the kind of thinking required when investigating breaks in slumping.

The split occurred before the slump was complete. We know this because the pieces no longer fit exactly together.  This means the crack opened as the slump continued.  There is other evidence.

The opening of the crack cannot have happened at or after the annealing. It would have already formed to the mould in a whole state. It would break completely across, because it would be in a brittle state.  And the pieces would fit exactly together.  But they do not.

This piece was at the bottom of a stack of shelves in a deep kiln.  At the bottom, there is no radiant heat, only side heat.  This could be a major cause the kind of break described.

It is possible that the split was not across the whole piece.  At the bottom of the kiln, the glass is not receiving any radiant heat from the top.  It is getting radiant heat only from the sides of the kiln.  That means the edges were considerably hotter than the centre.  The edge may be in a plastic state while the centre is still in the brittle state.  The contrasts in expansions are often great enough to break a piece.

From the evidence we have, it can only be said the ramp rate was too fast for the conditions. 

This little exercise shows that a lot of information about layup, schedule, place in the kiln, and any other relevant variation on the usual, must be detailed when asking why something has not turned out as expected. 

 

 

Wednesday 10 July 2024

Uneven Slumps on Deep Rectangular Moulds

 "Can anyone please tell me why this mould always comes out wonky and devitrifies and pulls in on the edges. I used Primo Primer; my kiln is level, and this is the slump schedule I use for 3mm base with 6mm in places [temperatures in Celsius]: 100/593/30 mins; 66/663/25 mins; 204/482/60 mins; 66/371/10 mins; END.*   12cm square."




The suggestion has been made that having a 6mm base would lessen the irregular slump in the mould.  I am not convinced that making the base thicker will sort the problems.

 

1)  This is a very deep mould in relation to the span.  The mould sides are steep.

 

2) The glass slides down and picks up marks from sliding down the walls of the mould.  The marks are not devitrification.

 

3) Deep slumps are prone to going off centre. One fix is to watch and be prepared to reach in with wet sticks to readjust the glass placement on the mould.  

 

4) Deep moulds (deep is relative to the span of the mould) require two or more stages of slumping. Start with shallow a slump, and progress through steeper ones.


5) The sides dog bone on many rectangular moulds.  One way to reduce this is to round the corners with a 10mm radius.

 

6) Reducing the forming temperature, and extending the soak time dramatically, will go some way to alleviating the previous problems. I suggest trying a 620C slump temperature and soak for 2 - 3 hours.  Peek at intervals to see when the slump is complete, then advance to anneal and cool.


In my view, it is a mould from a maker that does not fully understand glass behaviour.

And in passing, the ramp speed from top temperature to annealing should be as fast as possible, to avoid any risk of devitrification on the way down.  

* Schedule in Fahrenheit for the Americans.  

  • 198 to 1100, 30' 
  • 119 to 1225, 25'
  • 367 to 900, 60'  [ASAP is the recommended rate.  As it is a tack fused piece, I would anneal as though 12mm/4 layers.  This would use a 2 hour soak, cool at 100 to 800, 180 to 700, off ]
  • 120 to 700, 10'
  • End

Wednesday 3 July 2024

Multiple Layers of Kiln Wash and Fibre

Recently, there have been confirmations of multiple of layers of kiln wash on the shelf under pot melts, frit stretches, and flows.  Ten, and even sixteen layers are mentioned. Also reported are two layers of 1mm fibre paper as a separator for the same processes.

These practices are excessive and wasteful.

 

Kiln wash   

·         Once fully covered, the shelf does not need additional layers. 

·         Stir the kiln wash mix each time you dip the brush.

·         Apply thinly.

·         Use only enough coats to evenly cover the shelf.

 

Fibre and shelf papers are not recommended to be placed on the shelf for high temperature processes.

·         The shelf papers can become incorporated within the glass as it moves along the shelf.

·         Fibre papers inhibit the movement of the glass in unpredictable ways.

 

If you do use fibre papers anyway:

·         Use only one layer.

·         Place a clear sheet of glass over the fibre paper to allow better flow during the firing.

·         A disc of clear glass also helps to separate opalescent glass from the shelf.

 

More layers of kiln wash or fibre paper does not make a better separator.


Wednesday 26 June 2024

Replacement Kiln Vent Plugs

 

Replacement Kiln Vent Plugs

Accidents happen.  Sometimes the lightweight plug for the vent of a kiln gets dropped and broken.  You can replace this, whether brick or ceramic.

A quick solution is to roll up some fibre blanket or thick fibre paper into a roll large enough to fit into the hole.  This is enough to keep the heat from escaping and stop outside air flowing in.  If you leave excess outside the plug hole, it allows you to pull it out and view the interior as usual.  This will last quite a while and can be renewed easily.

A more permanent solution is to shape soft fire brick.  This can be shaped with a cheap saw. The brick is soft but very abrasive. So, use a cheap saw or an old one.  I keep an old saw especially for shaping bricks and vermiculite.  You could use 50mm/2 inch vermiculite in this way too, but firebrick this thick or more is easy to obtain.

Cut a cube from a fire brick.  This usually is about one third of a full brick.




Mark all around with a pencil how thick the shoulder (the outer part of the plug) should be. 25mm or 1 inch is thick enough.  It is possible to have it thicker if you wish.  The important element is that the outside part of the plug should not over balance the neck that fits into the vent channel.

Present the brick to the vent hole and twist a little, this will leave a mark to determine the diameter required. Alternatively, measure the inside diameter and draw this onto the end of the brick with a soft pencil or charcoal.

One end of brick cube marked, although a little off centre

Saw down to the shoulder mark on each of the four corners. Then make it eight corners. Test how well this adjustment fits to the hole.  It is probable that it is too big on the corners, but ok on the flat sides.

The first four corners sawn off to the shoulder



This is the time to use a wood rasp to round the multiple corners. Repeat the testing for size and adjusting until the plug fits the hole.  



The plug should not be tight.  It needs only a loose fitting so that it is easy to remove and put in.

Fit too tight to slide easily into the vent.

Finally, with 60 grit sandpaper round off any remaining corners.  Test and sand more off until it slides easily into the hole. This should not take more than a quarter of an hour to complete.

 

Fit just right. It slides in and out easily.


Wednesday 19 June 2024

Slumping Breaks on “go-to” Schedules

 An "It has always worked for me before" schedule implies a single approach to slumping regardless of differing conditions.  Layup alterations, thickness variations, colour contrasts, mould variations all affect the scheduling.  The schedule for each piece needs to be altered when there are changes from the schedule for the “standard” piece, or mould.

Photo credit: Emma Lee


In the example shown, we are not told the schedule, but it shows that the rate was a little too fast. If it had been faster the glass would have separated further apart. The heat was enough to appear to recombine at the edges where it was not slumping so much. 

Review your "go to" schedules whenever something changes. It may still be a good base from which to work. But you need to assess the layup, thickness, and any other variations to help adjust the schedule to fire each piece.

Some of the variations from the “standard” to be considered are:

Single layer slumping 

Weight

Mould sizes

Relative Slumping Depth

Mould shape and detail


Wednesday 12 June 2024

How Many Times Can You Fuse?

Is there a limit to how often a piece can be refused either to add on new pieces or to break up and reuse?

 

Bullseye test their glass to ensure it can go through three firings.  After that you are on your own.  This limitation has been generally accepted within the kilnforming community.

Multiple Firings

Many people report that they fire their glass many times.  I have fired Bullseye glass up to seven times using powders.  The first five firings were to contour fuse.  The final fuse firing was to full fuse.  And then there was a slump firing to make up the seven firings.  These multiple firings assume that the temperature is not taken above full fuse for any of the firings.  The annealing for each of these firings remains as for the calculated thickness of the piece.  No additional annealing time is required for multiple firings without significant changes.

You do not need to consider firing multiple process at once.  The possible number of firings is more than enough to achieve multiple processes.

High Temperature Work

However, the many firings of my piece would not have been possible with high temperatures or long soaks.  The high temperature firings are those that go to casting temperatures (835ºC/1540ºF) and above. These are temperatures for things like pattern bars, melts, and castings.  The glass can change its nature enough to give problems at these temperatures, especially with long soaks.  

If you do multiple firings at high temperatures, I recommend annealing to be from one and a half to two times the expected thickness.  And the rate of cooling will need to be in line with the length of the anneal soak.

Even with care, there can be problems.  I created a thick bowl from transparent glass, of which I was proud.  After an afternoon in the sun while on display months later it showed a crack developing.  I am still convinced - by other similar work surviving – that I annealed it properly. It exhibited minimum stress after the final flat full fuse firing. It was not checked after the slump.

Multiple firings of items with soaks at high temperatures are less likely to survive.  The number of firings possible can be determined only by experience.

Wednesday 5 June 2024

Diagnosing Slump fractures

Once you have an initial idea of the source of the problem, think about it.  Test it against the evidence.  Is there enough evidence to make a call?  Make sure you have considered alternative explanations.  It is just too easy to make a snap decision about causes in low temperature processes.  The source of breaks in slumping are most often complex and stem from interrelated factors.

I give you an example of the difficulties of diagnosing a slumping break.

On a Facebook group a person showed the break of a single layer on a cyclone mould.  Others commented the same had happened to them.


Picture credit: Esther Mulvihill Pickens

Possible causes suggested on Facebook included:

  • Thermal shock on the way up
  • Thermal shock on the way down
  • Too large on the mould and broke due to differential contraction
  • Too many holds on the way up
  • Too hot
  • Too thin
  • Follow the CPI programme
  • Glass extending over the sides

Some of these suggestions were of general applicability, some in relation to the state of the broken glass.

The suggestions did not include:

  • Cause of the rounded dots at the bottom of the mould.
  • A cause for the state of the flat piece off the mould (it appears sharp edged.  Does it show some forming already?).
  • The cause for the location of the fully formed remaining glass.
  • The effect of the location of the mould and glass in the kiln.
  • The consequences of a short soak at top temperature. 
  • Is the kiln running hotter than most (1290ºF/698ºC for 10 minutes at top temperature was used)?

Of course, it is difficult to diagnose a problem from just one picture. It is difficult even with many pictures. And so, without handling the object, only suggestions can be made.

But….

You must spend enough time examining the piece with whatever other information is available to make specific suggestions.  The first thought may not consider all the factors.  Consider what kinds of causes there are for breaks during or after slumping.

More close inspection reveals the rounded edges of the break.  That supports the idea that the temperature was too high. It also supports the diagnosis that the break occurred on the heat up.

The edges of the piece that has fallen off the mould, and now rests on the shelf, seem to be square or sharp. This shows the extent of the difference of temperature between shelf and top of the mould – less than 100mm/4 inches.  Also, how small the differences in temperature are between slump and tack.  The extent of difference in fusing does depend on how high in the kiln the mould is placed.  That is demonstrated here by the different elevation of the two pieces. 

The conformation of the glass to the mould is complete.  This supports the diagnosis of the break occurring early in the firing, and certainly before the slump was complete.  These pieces will not fit together.  So, even if the edges were sharp the fact they will not fit together shows they conformed independently to the mould surface.  Therefore, the break was before forming temperature was reached.

The glass hangs over the mould edges on only three sides and at an angle.  This indicates the cause of the overhang was the break.  Not the reverse. An overhang at the beginning of the slump is likely to be even.

The piece on the floor of the kiln combined with the movement of the glass toward the back gives an indication that the origin of the break is at the front.  This relates to uneven temperatures and to the placement of the mould.

No one mentioned the placement of the mould and glass at the back of the kiln.  This will have an effect on scheduling.  The mould and glass are very large in relation to the kiln.  There is little space between the glass on the mould and the walls of the kiln.  Also, the mould is placed asymmetrically in the kiln – very close on three sides.  This will cause uneven heating in any kiln.  To have a successful firing of glass on this mould in this kiln will require radically different schedules to that for a centrally placed mould that is moderate for the size of the kiln.

The large size (relative to the kiln) and the asymmetrical placing are the causes of the break, in my opinion.  I admit that it took me several looks to realise the placement was a key cause of the break.

So, the generalised comments about thermal shock are correct, but not as to the cause of that shock.  The kiln will be hotter in the central part and cooler at the corners.  This is true of all rectangular kilns.  The important thing is to learn how to cope with these temperature differences.

Slow firings to low temperatures with long soaks are the three important elements.  These make up the heat work of the kiln. Applying this to a schedule means:

  • slow ramp up rates – as little as one half the recommended rates for centrally placed moulds that are moderately sized in relation to the kiln.
  • Low temperatures present lesser risks to the control of the outcome of the firing.  Determining the lower temperature possible requires peeking into the kiln to monitor the progress of the firing.
  • Long soaks combined with low temperatures get the kilnforming done with minimal marking of the underside.  Low temperature soaks - in excess of 30 minutes - are required to minimise the marking.  Observation of the slump will be necessary to determine when it is complete.

My suggestions for the causes of other elements are:

·        Cause of the rounded dots at the bottom of the mould.

The temperature was too high. 698ºC/1290ºF is much hotter than needed for a slump. It was hot enough to round edges and small shards of glass.  Which shows excessive heat was received by the glass.

·        A cause for the state of the flat piece off the mould (it appears sharp edged. Does it show some forming already?)

The soak of 10 minutes was too short for the temperature in the kiln to equalise from top to bottom.  The glass on the shelf may not have reached 650ºC/1200ºF with such a short soak.

·        The cause for the location of the fully formed remaining glass.

The glass broke and was forced apart by the size of the expansion differences within the glass.  The movement of a piece at the front of the mould combined with the rearward and side movement of the glass indicate the origin of the break was at the front.  The distance apart shows the amount of force, and so the degree of reduction in the ramp rate required to fire this successfully.

·        The effect of the location of the mould and glass in the back of the kiln has already been discussed.

·         The consequences of a short soak at top temperature.

A high temperature is often considered necessary to pick up all the detail in moulds, whether slump or texture moulds.  The same effect can be achieved at lower temperatures with longer soaks.  The results of this strategy are fewer mould marks on the bottom of the work.

·        Is the kiln running hotter than most (Used 1290F/698C for 10 minutes at top temperature)?

This is one that cannot be answered other than by experiments carried out by the owner of the kiln.  Look at the Bullseye Tech Note #1 Knowing your Kiln for methods of testing temperatures. 

In short:

Diagnosis of slumping breaks is more complex than it appears at first.


More information is available in the eBook Low Temperature Kilnforming, an Evidence Based Approach to Scheduling.

This is available from Bullseye or Etsy


Wednesday 29 May 2024

Draping Different Thicknesses and Sizes




Scheduling for different sizes and thicknesses of drapes requires schedules specific to these factors in addition to observing the progress of the drape.

Bob Leatherbarrow's research shows 6mm drapes more slowly than 3mm. It seems the thicker glass takes longer to begin the slump.  Glass behaves in a similar way for a drape.  My experience of draping 6mm/0.25” and 3mm/0.125” in the same firing confirms that 6mm takes longer.  Or, it needs a higher temperature.  I know this goes against common sense, but tests and experience show it to be true.

If you try to drape 3mm/0.125” and 6mm/0.25” pieces at the same time, the 3mm will reach the desired shape before the 6mm. You then have the choice of an under draped 6mm piece or an over draped 3mm piece.  This indicates that draping different thicknesses in the same firing will be unsuccessful.  To a lesser extent, the size of the drape will influence the speed of the drop.  So, you are unlikely to achieve completely desirable results with significantly different sizes of drape in the same firing either.

Observation is essential in all draping operations. You cannot know how long it will take for a piece to drape or drop to your requirements.  To be sure of your result you need to observe the progress of the drape.  There is rarely a safety net of a form to drape onto as in slumping.  To observe, set your top temperature with a long soak/hold.  Start peeking at frequent intervals from the time top temperature is reached.  

When the glass has reached the desired shape, advance to the next segment.  Your controller manual will give you instructions on how to do that.

Different thickness and sizes of glass require different firing conditions.

Wednesday 22 May 2024

Slumping and Annealing bottles



"Can a tack fuse schedule for fusing glass can be used to slump bottles?"

It may be that this person does not have the confidence to write a new schedule.  They may wish to use an existing schedule for another purpose. The short answer is “Although a Bullseye or Oceanside tack fuse temperature will be high enough to slump bottles, they are not suitable for annealing”.  There are reasons for this. 

The softening point of float glass, which is similar to bottle glass, is 720ºC/1330ºF.  Slumping would normally be done at about 20ºC/36ºF above this. You also need a slumping hold at this temperature much longer than a tack fuse schedule would use.

if you use a tack fuse schedule for a fusing glass, your annealing will be inadequate. Bottle and float glass tend to have an annealing point of around 540ºC/1005ºF. An annealing for fusing glass will be between 515ºC/960ºF and 482ºC/900ºF.  This is likely to be too low an annealing point for bottles.  Also, the annealing soak is likely to be too short. Slumped bottles are very thick at the base where it folds over the cylinder of the bottle.  This requires a longer anneal soak and slower cool than a schedule for a tack fuse of fusing glass.

Checking for stress in the completed work is normal.  It is essential for your finished bottle if you use a tack fuse to fire it.

 